MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Plaskolite Optix® Acrylic Sheet
Categories: Polymer; Thermoplastic; Acrylic (PMMA); Acrylic, Optical Sheet

Material Notes: Optix® is a continuously processed acrylic sheet that is crystal clear, impact resistant, weather resistant, and non-yellowing. It offers high molecular weight for superior thermoforming, bending, and flame polishing.

Data provided by the manufacturer, Plaskolite, Inc.

Key Words: PMMA; Polymethyl Methacrylate
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.19 g/cc0.0430 lb/in³ASTM D792
Water Absorption 0.40 %0.40 %ASTM D570
Linear Mold Shrinkage 0.0040 cm/cm0.0040 in/inShrinkage; ASTM D702
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 93930.64 cm sample; ASTM D785
Tensile Strength, Yield 70.0 MPa10200 psiASTM D638
Elongation at Break 5.1 %5.1 %ASTM D638
Tensile Modulus 3.00 GPa435 ksiASTM D638
Flexural Yield Strength 101 MPa14600 psiASTM D790
Izod Impact, Notched 0.400 J/cm0.749 ft-lb/inMolded Notch
 0.200 J/cm
@Temperature -18.0 °C
0.375 ft-lb/in
@Temperature -0.400 °F
ASTM D256
Gardner Impact 0.450 J0.332 ft-lbJ; ASTM D3029-GB, unpainted
Tensile Impact Strength 42.0 kJ/m²20.0 ft-lb/in²ASTM D1822
Abrasion 5050% haze after 200 cycles per ASTM D1044
 
Thermal PropertiesMetricEnglishComments
CTE, linear 52.2 µm/m-°C
@Temperature -18.0 - 38.0 °C
29.0 µin/in-°F
@Temperature -0.400 - 100 °F
ASTM D696
Thermal Conductivity 0.130 W/m-K0.902 BTU-in/hr-ft²-°FASTM C177
Melting Point 149 - 157 °C300 - 315 °F
Maximum Service Temperature, Air 77.0 - 88.0 °C171 - 190 °FContinuous Service
Deflection Temperature at 0.46 MPa (66 psi) 96.0 °C205 °F2°C/min unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 88.0 °C190 °F2°C/min (3.6°F/min) unannealed; ASTM D648
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.461.46ASTM D542
Haze 2.0 %
@Thickness 2.50 mm
2.0 %
@Thickness 0.0984 in
ASTM D1003
Transmission, Visible 92 %92 %ASTM D1003

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Röhm Plexiglas® 99560 Superclear Extruded PMMA Sheet
SEKISUI SPI KYDEX® 5555 Acrylic/PVC
LG Chemical IH830 PMMA, General Purpose Grade for Injection Molding
Overview of materials for PVC, Molded
Röhm Plexiglas® GS 0F00 (233) Cast Acrylic

PPLAS6 / 56279

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.