MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

BASF Capron® 8202 NL Nylon 6 (Dry)  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced

Material Notes: Capron 8202 NL is an unfilled, low viscosity, non-lubricated nylon 6 injection molding homopolymer exhibiting excellent melt fluidity for filling thin sections. It is available in natural, heat stabilized and pigmented versions. It combines good strength, stiffness, and toughness as well as excellent heat, chemical and abrasion resistance.

Capron 8202 NL is generally recommended for applications such as: gears, fittings, casters, bearings, clips, fasteners, plugs, caps, and filter bowls.

Data provided by Allied Signal.

Processing: Max. water content 0.25%. Product is supplied in sealed containers and drying is not required. If drying becomes necessary, a dehumidifying or desiccant dryer operating at 85°C (185 °F). Is recommended. Drying time is dependent on moisture level.

Melt Temperature: 240-280 degC (464-536 degF). Mold Temperature: 80-95 degC (176-203 degF). Injection and Packing Pressure: 35-125 bar (500-1500psi) A mold temperature of 80-95 degC (176-203 degF) is recommended, but temperatures of as low as 10 degC (50 degF) can be used where applicable. Injection pressure controls the filling of the part and should be applied for 90% of ram travel. Packing pressure affects the final part and can be used effectively in controlling sink marks and shrinkage. It should be applied and maintained until the gate area is completely frozen off. Fast fill rates are recommended to insure uniform melt delivery to the cavity and prevent premature freezing.

Capron® is no longer a part of the BASF standard line. The BASF nylon products have been consolidated in the Ultramid ® line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.13 g/cc0.0408 lb/in³ISO data
Water Absorption 1.6 %1.6 %24 hrs; ISO data
Moisture Absorption at Equilibrium 2.7 %2.7 %50% RH; 23°C; ISO data
Water Absorption at Saturation 9.5 %9.5 %in water; 23°C; ISO data
Viscosity Measurement 4848Formic Acid Viscosity; ISO data
Linear Mold Shrinkage 0.012 cm/cm0.012 in/inASTM Data MD
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 75.0 MPa10900 psiASTM data at 5 mm/min.
Tensile Strength, Yield 80.0 MPa11600 psiASTM value at 50 mm/min.
 82.0 MPa11900 psiISO value at 50 mm/min.
Elongation at Break >= 50 %>= 50 %Nominal
 55 %55 %Nominal
Elongation at Yield 4.0 %4.0 %ASTM Value at 50 mm/min.
 4.0 %4.0 %ISO Value at 50 mm/min.
Tensile Modulus 3.10 GPa450 ksisame value from ASTM and ISO test.
Flexural Yield Strength 110 MPa16000 psiASTM Data
Flexural Modulus 2.83 GPa410 ksiASTM Data
Poissons Ratio 0.350.35ISO data
Shear Modulus 1.10 GPa160 ksicalculated
 
Thermal PropertiesMetricEnglishComments
CTE, linear 83.0 µm/m-°C
@Temperature 20.0 °C
46.1 µin/in-°F
@Temperature 68.0 °F
ASTM data
Melting Point 220 °C428 °FASTM and ISO test
Deflection Temperature at 0.46 MPa (66 psi) 178 °C352 °FValue for both ASTM and ISO data.
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °C140 °FISO data
 65.0 °C149 °FASTM Data
 
Processing PropertiesMetricEnglishComments
Drying Temperature 85.0 °C185 °FSee Materials Notes

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Capron® 8202C HS Nylon 6 (Conditioned)
Domo Technyl® C206F Unfilled, Fast Cycle Nylon 6
BASF Ultramid® 8202 PA6 (Dry)
A. Schulman SCHULAMID® 6 MV14 Unreinforced Nylon 6
BASF Capron® B100QP Nylon 6 (DAM)

PALC29 / 23823

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.