Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Overview of materials for Polycarbonate/ABS Alloy, Unreinforced
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced; Polycarbonate (PC)

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polycarbonate/ABS Alloy, Unreinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.960 - 1.50 g/cc0.0347 - 0.0542 lb/in³Average value: 1.16 g/cc Grade Count:1105
 0.935 - 1.01 g/cc
@Temperature 240 - 260 °C
0.0338 - 0.0365 lb/in³
@Temperature 464 - 500 °F
Average value: 0.981 g/cc Grade Count:10
Filler Content 10.0 %10.0 %Average value: 10.0 % Grade Count:3
Volatile Organic Compounds (VOC) Content 9.00 - 15.0 g/l9.00 - 15.0 g/lAverage value: 11.1 g/l Grade Count:10
Water Absorption 0.0100 - 0.700 %0.0100 - 0.700 %Average value: 0.295 % Grade Count:305
Moisture Absorption at Equilibrium 0.0100 - 0.900 %0.0100 - 0.900 %Average value: 0.162 % Grade Count:244
Water Absorption at Saturation 0.110 - 1.00 %0.110 - 1.00 %Average value: 0.555 % Grade Count:118
Viscosity 105000 - 211000 cP
@Temperature 260 - 260 °C
105000 - 211000 cP
@Temperature 500 - 500 °F
Average value: 141000 cP Grade Count:4
 8.00 - 41.0 cP
@Temperature 260 - 265 °C
8.00 - 41.0 cP
@Temperature 500 - 509 °F
Average value: 141000 cP Grade Count:33
 8.00 - 41.0 cP
@Load 2.16 - 10.0 kg
8.00 - 41.0 cP
@Load 4.76 - 22.0 lb
Average value: 141000 cP Grade Count:33
 150000 - 520000 cP
@Temperature 260 - 260 °C
150000 - 520000 cP
@Temperature 500 - 500 °F
Average value: 141000 cP Grade Count:12
 150000 - 520000 cP
@Frequency 1000 - 1000 Hz
150000 - 520000 cP
@Frequency 1000 - 1000 Hz
Average value: 141000 cP Grade Count:12
 170 - 2.00e+6 cP
@Temperature 260 - 260 °C
170 - 2.00e+6 cP
@Temperature 500 - 500 °F
Average value: 141000 cP Grade Count:38
 170 - 2.00e+6 cP
@Shear Rate 1000 - 1500 1/s
170 - 2.00e+6 cP
@Shear Rate 1000 - 1500 1/s
Average value: 141000 cP Grade Count:38
Maximum Moisture Content 0.0100 - 0.05000.0100 - 0.0500Average value: 0.0218 Grade Count:74
Linear Mold Shrinkage 0.000600 - 0.0800 cm/cm0.000600 - 0.0800 in/inAverage value: 0.00565 cm/cm Grade Count:833
 0.00700 - 0.00700 cm/cm
@Temperature 80.0 - 80.0 °C
0.00700 - 0.00700 in/in
@Temperature 176 - 176 °F
Average value: 0.00700 cm/cm Grade Count:3
Linear Mold Shrinkage, Transverse 0.000600 - 0.0100 cm/cm0.000600 - 0.0100 in/inAverage value: 0.00564 cm/cm Grade Count:223
 0.00700 - 0.00700 cm/cm
@Temperature 80.0 - 80.0 °C
0.00700 - 0.00700 in/in
@Temperature 176 - 176 °F
Average value: 0.00700 cm/cm Grade Count:3
Melt Flow 0.400 - 95.0 g/10 min0.400 - 95.0 g/10 minAverage value: 18.5 g/10 min Grade Count:945
Spiral Flow 25.0 - 76.0 cm9.84 - 29.9 inAverage value: 52.6 cm Grade Count:17
 47.0 - 58.0 cm
@Temperature 260 - 260 °C
18.5 - 22.8 in
@Temperature 500 - 500 °F
Average value: 47.2 cm Grade Count:4
 24.7 - 63.0 cm
@Temperature 260 - 260 °C
9.72 - 24.8 in
@Temperature 500 - 500 °F
Average value: 47.2 cm Grade Count:5
 24.7 - 63.0 cm
@Thickness 2.00 - 2.00 mm
9.72 - 24.8 in
@Thickness 0.0787 - 0.0787 in
Average value: 47.2 cm Grade Count:5
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 72.0 - 97.072.0 - 97.0Average value: 90.4 Grade Count:8
Hardness, Rockwell R 98.0 - 12398.0 - 123Average value: 115 Grade Count:297
Hardness, Shore A 45.0 - 85.045.0 - 85.0Average value: 63.2 Grade Count:11
Hardness, Shore D 62.0 - 85.062.0 - 85.0Average value: 70.7 Grade Count:6
Hardness, Shore M 30.0 - 95.030.0 - 95.0Average value: 55.0 Grade Count:3
Ball Indentation Hardness 12.0 - 126 MPa1740 - 18300 psiAverage value: 98.2 MPa Grade Count:25
Tensile Strength, Ultimate 2.80 - 586 MPa406 - 85000 psiAverage value: 53.3 MPa Grade Count:568
 20.0 - 45.0 MPa
@Temperature 60.0 - 90.0 °C
2900 - 6530 psi
@Temperature 140 - 194 °F
Average value: 32.5 MPa Grade Count:1
Tensile Strength, Yield 5.00 - 119 MPa725 - 17300 psiAverage value: 56.3 MPa Grade Count:826
Elongation at Break 0.800 - 1230 %0.800 - 1230 %Average value: 68.9 % Grade Count:813
 45.0 - 55.0 %
@Temperature 60.0 - 90.0 °C
45.0 - 55.0 %
@Temperature 140 - 194 °F
Average value: 50.0 % Grade Count:1
Elongation at Yield 1.90 - 80.0 %1.90 - 80.0 %Average value: 5.48 % Grade Count:363
 4.00 - 6.00 %
@Temperature 60.0 - 90.0 °C
4.00 - 6.00 %
@Temperature 140 - 194 °F
Average value: 5.00 % Grade Count:1
Modulus of Elasticity 1.67 - 11.1 GPa242 - 1610 ksiAverage value: 2.60 GPa Grade Count:510
 1.90 - 2.20 GPa
@Temperature 60.0 - 90.0 °C
276 - 319 ksi
@Temperature 140 - 194 °F
Average value: 2.05 GPa Grade Count:1
Flexural Yield Strength 8.20 - 900 MPa1190 - 131000 psiAverage value: 88.1 MPa Grade Count:798
Flexural Modulus 0.290 - 23.1 GPa42.1 - 3350 ksiAverage value: 2.57 GPa Grade Count:899
Flexural Strain at Break 1.30 - 6.10 %1.30 - 6.10 %Average value: 4.15 % Grade Count:4
Compressive Yield Strength 53.0 - 170 MPa7690 - 24700 psiAverage value: 84.5 MPa Grade Count:6
Bearing Yield Strength 25.2 - 293 MPa3650 - 42500 psiAverage value: 134 MPa Grade Count:5
Poissons Ratio 0.340 - 0.3800.340 - 0.380Average value: 0.353 Grade Count:9
Shear Strength 40.3 - 61.9 MPa5850 - 8980 psiAverage value: 54.3 MPa Grade Count:5
Izod Impact 37.0 - 824 J27.3 - 608 ft-lbAverage value: 511 J Grade Count:50
 37.0 - 480 J
@Temperature -30.0 - -30.0 °C
27.3 - 354 ft-lb
@Temperature -22.0 - -22.0 °F
Average value: 172 J Grade Count:31
Izod Impact, Notched 0.196 - 56.0 J/cm0.367 - 105 ft-lb/inAverage value: 5.31 J/cm Grade Count:625
 0.600 - 6.40 J/cm
@Temperature -50.0 - 0.000 °C
1.12 - 12.0 ft-lb/in
@Temperature -58.0 - 32.0 °F
Average value: 3.48 J/cm Grade Count:115
 1.01441 - 5.34 J/cm
@Temperature -40.0 - 0.000 °C
1.90041 - 10.0 ft-lb/in
@Temperature -40.0 - 32.0 °F
Average value: 3.48 J/cm Grade Count:49
 1.01441 - 5.34 J/cm
@Thickness 3.17 - 6.35 mm
1.90041 - 10.0 ft-lb/in
@Thickness 0.125 - 0.250 in
Average value: 3.48 J/cm Grade Count:49
Izod Impact, Unnotched 0.530 J/cm - NB0.993 ft-lb/in - NBAverage value: 7.05 J/cm Grade Count:84
 2.00 J/cm - NB
@Temperature -30.0 - 0.000 °C
3.75 ft-lb/in - NB
@Temperature -22.0 - 32.0 °F
Average value: 4.66 J/cm Grade Count:16
Izod Impact, Notched (ISO) 1.80 - 80.0 kJ/m²0.857 - 38.1 ft-lb/in²Average value: 38.7 kJ/m² Grade Count:272
 4.00 - 61.0 kJ/m²
@Temperature -40.0 - 0.000 °C
1.90 - 29.0 ft-lb/in²
@Temperature -40.0 - 32.0 °F
Average value: 22.3 kJ/m² Grade Count:159
 15.0 - 35.7 kJ/m²
@Temperature -30.0 - -30.0 °C
7.14 - 17.0 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 22.3 kJ/m² Grade Count:2
 15.0 - 35.7 kJ/m²
@Thickness 3.17 - 3.20 mm
7.14 - 17.0 ft-lb/in²
@Thickness 0.125 - 0.126 in
Average value: 22.3 kJ/m² Grade Count:2
Izod Impact, Unnotched (ISO) 3.00 kJ/m² - NB1.43 ft-lb/in² - NBAverage value: 52.1 kJ/m² Grade Count:86
 21.0 kJ/m² - NB
@Temperature -30.0 - -30.0 °C
9.99 ft-lb/in² - NB
@Temperature -22.0 - -22.0 °F
Average value: 109 kJ/m² Grade Count:38
Charpy Impact Unnotched 0.290 J/cm² - NB1.38 ft-lb/in² - NBAverage value: 9.66 J/cm² Grade Count:180
 3.50 J/cm² - NB
@Temperature -40.0 - -20.0 °C
16.7 ft-lb/in² - NB
@Temperature -40.0 - -4.00 °F
Average value: 16.8 J/cm² Grade Count:54
Charpy Impact, Notched 0.0900 - 11.0 J/cm²0.428 - 52.4 ft-lb/in²Average value: 3.98 J/cm² Grade Count:330
 0.500 - 6.00 J/cm²
@Temperature -40.0 - 0.000 °C
2.38 - 28.6 ft-lb/in²
@Temperature -40.0 - 32.0 °F
Average value: 2.23 J/cm² Grade Count:175
 3.57 - 3.57 J/cm²
@Temperature -30.0 - -30.0 °C
17.0 - 17.0 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 2.23 J/cm² Grade Count:1
 3.57 - 3.57 J/cm²
@Thickness 3.20 - 3.20 mm
17.0 - 17.0 ft-lb/in²
@Thickness 0.126 - 0.126 in
Average value: 2.23 J/cm² Grade Count:1
Gardner Impact 4.52 - 71.4 J3.33 - 52.7 ft-lbAverage value: 38.3 J Grade Count:37
 59.0 - 59.0 J
@Temperature -29.0 - -29.0 °C
43.5 - 43.5 ft-lb
@Temperature -20.2 - -20.2 °F
Average value: 65.7 J Grade Count:2
Dart Drop, Total Energy 11.0 - 90.0 J8.11 - 66.4 ft-lbAverage value: 54.2 J Grade Count:100
 8.00 - 90.0 J
@Temperature -30.0 - -28.9 °C
5.90 - 66.4 ft-lb
@Temperature -22.0 - -20.0 °F
Average value: 53.3 J Grade Count:33
 56.5 - 59.9 J
@Temperature -29.0 - -29.0 °C
41.7 - 44.2 ft-lb
@Temperature -20.2 - -20.2 °F
Average value: 53.3 J Grade Count:2
 56.5 - 59.9 J
@Thickness 3.20 - 3.20 mm
41.7 - 44.2 ft-lb
@Thickness 0.126 - 0.126 in
Average value: 53.3 J Grade Count:2
Falling Dart Impact 6.78 - 60.0 J5.00 - 44.3 ft-lbAverage value: 41.3 J Grade Count:8
 50.1653 - 50.1653 J
@Temperature -28.9 - -28.9 °C
37.0000 - 37.0000 ft-lb
@Temperature -20.0 - -20.0 °F
Average value: 50.2 J Grade Count:1
Instrumented Impact Total Energy 4.00 - 62.2 J2.95 - 45.9 ft-lbAverage value: 49.3 J Grade Count:16
Puncture Energy 44.0 - 51.0 J32.5 - 37.6 ft-lbAverage value: 46.3 J Grade Count:6
 20.0 - 57.0 J
@Temperature -30.0 - -30.0 °C
14.8 - 42.0 ft-lb
@Temperature -22.0 - -22.0 °F
Average value: 47.0 J Grade Count:6
Coefficient of Friction 0.160 - 0.3700.160 - 0.370Average value: 0.246 Grade Count:7
Coefficient of Friction, Static 0.0500 - 0.1800.0500 - 0.180Average value: 0.142 Grade Count:5
Tensile Creep Modulus, 1 hour 1800 - 2500 MPa261000 - 363000 psiAverage value: 2140 MPa Grade Count:5
Tensile Creep Modulus, 1000 hours 1500 - 1900 MPa218000 - 276000 psiAverage value: 1720 MPa Grade Count:5
K (wear) Factor 14.1 - 2520 x 10-8 mm³/N-M7.00 - 1250 x 10-10 in³-min/ft-lb-hrAverage value: 754 x 10-8 mm³/N-M Grade Count:4
Taber Abrasion, mg/1000 Cycles 54.0 - 82.054.0 - 82.0Average value: 64.4 Grade Count:7
Compression Set 21.0 - 45.0 %21.0 - 45.0 %Average value: 32.3 % Grade Count:11
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 100 - 1.00e+18 ohm-cm100 - 1.00e+18 ohm-cmAverage value: 4.91e+16 ohm-cm Grade Count:297
Surface Resistance 10.0 - 5.00e+17 ohm10.0 - 5.00e+17 ohmAverage value: 1.08e+16 ohm Grade Count:278
Static Decay 0.0100 - 0.250 sec0.0100 - 0.250 secAverage value: 0.0580 sec Grade Count:5
Shielding Effectiveness 47.0 - 70.0 dB47.0 - 70.0 dBAverage value: 54.9 dB Grade Count:3
Dielectric Constant 2.00 - 3.402.00 - 3.40Average value: 2.93 Grade Count:166
Dielectric Strength 2.76 - 70.0 kV/mm70.0 - 1780 kV/inAverage value: 28.1 kV/mm Grade Count:222
Dissipation Factor 0.00100 - 0.01500.00100 - 0.0150Average value: 0.00588 Grade Count:150
Arc Resistance 60.0 - 180 sec60.0 - 180 secAverage value: 112 sec Grade Count:51
Comparative Tracking Index 175 - 650 V175 - 650 VAverage value: 331 V Grade Count:183
Hot Wire Ignition, HWI 7.00 - 120 sec7.00 - 120 secAverage value: 42.5 sec Grade Count:60
High Amp Arc Ignition, HAI 30.0 - 120 arcs30.0 - 120 arcsAverage value: 108 arcs Grade Count:52
High Voltage Arc-Tracking Rate, HVTR 25.4 - 150 mm/min1.00 - 5.91 in/minAverage value: 115 mm/min Grade Count:20
 
Thermal PropertiesMetricEnglishComments
CTE, linear 7.00 - 110 µm/m-°C3.89 - 61.1 µin/in-°FAverage value: 71.0 µm/m-°C Grade Count:353
 -60.0 - 74.0 µm/m-°C
@Temperature 29.0 - 100 °C
-33.3 - 41.1 µin/in-°F
@Temperature 84.2 - 212 °F
Average value: 17.1 µm/m-°C Grade Count:5
CTE, linear, Transverse to Flow 8.00 - 105 µm/m-°C4.44 - 58.3 µin/in-°FAverage value: 74.6 µm/m-°C Grade Count:197
 8.30 - 80.0 µm/m-°C
@Temperature 40.0 - 100 °C
4.61 - 44.4 µin/in-°F
@Temperature 104 - 212 °F
Average value: 32.2 µm/m-°C Grade Count:3
Specific Heat Capacity 1.23 - 2.54 J/g-°C0.294 - 0.607 BTU/lb-°FAverage value: 1.78 J/g-°C Grade Count:16
Thermal Conductivity 0.142 - 1.70 W/m-K0.985 - 11.8 BTU-in/hr-ft²-°FAverage value: 0.222 W/m-K Grade Count:68
 0.240 - 0.260 W/m-K
@Temperature 30.0 - 280 °C
1.67 - 1.80 BTU-in/hr-ft²-°F
@Temperature 86.0 - 536 °F
Average value: 0.250 W/m-K Grade Count:2
Melting Point 130 - 270 °C266 - 518 °FAverage value: 219 °C Grade Count:6
Maximum Service Temperature, Air 60.0 - 132 °C140 - 270 °FAverage value: 103 °C Grade Count:45
Hot Ball Pressure Test 75.0 - 125 °C167 - 257 °FAverage value: 94.3 °C Grade Count:84
Deflection Temperature at 0.46 MPa (66 psi) 53.9 - 250 °C129 - 482 °FAverage value: 112 °C Grade Count:504
Deflection Temperature at 1.8 MPa (264 psi) 52.0 - 160 °C126 - 320 °FAverage value: 101 °C Grade Count:929
Vicat Softening Point 38.1 - 230 °C101 - 446 °FAverage value: 117 °C Grade Count:628
 97.0 - 136 °C
@Temperature 50.0 - 50.0 °C
207 - 277 °F
@Temperature 122 - 122 °F
Average value: 119 °C Grade Count:8
 97.0 - 136 °C
@Load 5.10 - 5.10 kg
207 - 277 °F
@Load 11.2 - 11.2 lb
Average value: 119 °C Grade Count:8
Minimum Service Temperature, Air -50.0 - -40.0 °C-58.0 - -40.0 °FAverage value: -41.3 °C Grade Count:15
Glass Transition Temp, Tg 94.0 - 161 °C201 - 322 °FAverage value: 123 °C Grade Count:12
UL RTI, Electrical 60.0 - 105 °C140 - 221 °FAverage value: 74.5 °C Grade Count:135
UL RTI, Mechanical with Impact 60.0 - 100 °C140 - 212 °FAverage value: 71.7 °C Grade Count:136
UL RTI, Mechanical without Impact 60.0 - 105 °C140 - 221 °FAverage value: 74.1 °C Grade Count:136
Flammability, UL94 HB - 5VAHB - 5VAGrade Count:785
Flame Spread 5.00 - 50.0 mm/min0.197 - 1.97 in/minAverage value: 25.2 mm/min Grade Count:5
Smoke Density 40.0 - 22540.0 - 225Average value: 138 Grade Count:3
Oxygen Index 20.0 - 35.0 %20.0 - 35.0 %Average value: 27.2 % Grade Count:92
Glow Wire Test 550 - 960 °C1020 - 1760 °FAverage value: 833 °C Grade Count:132
 
Optical PropertiesMetricEnglishComments
Gloss 2.50 - 105 %2.50 - 105 %Average value: 55.3 % Grade Count:11
Transmission, Visible 0.100 - 93.0 %0.100 - 93.0 %Average value: 23.4 % Grade Count:3
 
Processing PropertiesMetricEnglishComments
Processing Temperature 60.0 - 302 °C140 - 575 °FAverage value: 205 °C Grade Count:131
Nozzle Temperature 220 - 330 °C428 - 626 °FAverage value: 261 °C Grade Count:280
Adapter Temperature 210 - 270 °C410 - 518 °FAverage value: 235 °C Grade Count:4
Die Temperature 210 - 265 °C410 - 509 °FAverage value: 241 °C Grade Count:6
Melt Temperature 180 - 330 °C356 - 626 °FAverage value: 255 °C Grade Count:588
Mold Temperature 26.7 - 150 °C80.0 - 302 °FAverage value: 72.9 °C Grade Count:619
Injection Velocity 40.0 - 240 mm/sec1.57 - 9.45 in/secAverage value: 237 mm/sec Grade Count:67
Roll Temperature 65.0 - 100 °C149 - 212 °FAverage value: 81.7 °C Grade Count:3
Drying Temperature 21.1 - 140 °C70.0 - 284 °FAverage value: 92.6 °C Grade Count:565
Moisture Content 0.0100 - 0.300 %0.0100 - 0.300 %Average value: 0.0331 % Grade Count:200
Dew Point -40.0 - -17.8 °C-40.0 - 0.000 °FAverage value: -28.9 °C Grade Count:14
Drying Air Flow Rate 22.7 - 28.3 l/min0.800 - 1.00 ft³/min (CFM)Average value: 25.5 l/min Grade Count:3
Injection Pressure 4.96 - 150 MPa720 - 21800 psiAverage value: 94.1 MPa Grade Count:69
Vent Depth 0.00300 - 0.00762 cm0.00118 - 0.00300 inAverage value: 0.00536 cm Grade Count:84
Cushion 0.330 - 0.635 cm0.130 - 0.250 inAverage value: 0.483 cm Grade Count:3
Precipitation Temperature 60.0 - 80.0 °C140 - 176 °FAverage value: 70.0 °C Grade Count:22

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
Overview of materials for Polycarbonate/ABS Alloy, Glass Fiber Filled
Overview of materials for Polycarbonate, Molded
Overview of materials for Polycarbonate/ABS Alloy, Carbon Fiber Filled
Overview of materials for PC/ABS + Stainless Steel

O1170a / 89060

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.