MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

ExxonMobil Optema® TC-114 Cast Ethylene Methyl Acrylate
Categories: Polymer; Film; Thermoplastic; Ethylene Methyl Acrylate; Ethylene-Methyl Acrylate Copolymer, Film Grade

Material Notes: Product Description: Optema TC 114 is an ethylene methyl acrylate copolymer specifically formulated to offer extrusion and property performance for blown and cast film applications. It produces a soft, elastic film with good handling characteristics without additional additives. Optema TC 114 can produce film under 1.0 mil thickness.

Availability: Latin America, North America and South America

Additive:

  • Anitblock: 14000 ppm
  • Slip: 3000 ppm
  • Thermal Stabilizer: Yes
Applications:
  • Disposable Gloves
  • Hospital Drapes
  • Upholstery Film

Data provided by the manufacturer, Exxon Chemical.

Key Words: EMA; Exxon Chemical Company
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.947 g/cc0.0342 lb/in³Exxon Method
Methyl Acrylate Content 18 %18 %Exxon Method
Thickness 31.8 microns1.25 mil
Melt Flow 3.2 g/10 min
@Load 2.16 kg,
Temperature 190 °C
3.2 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
Antiblock Level 1400 ppm1400 ppm
Slip Level 3000 ppm3000 ppm[ppm]
 
Mechanical PropertiesMetricEnglishComments
Film Elongation at Break, MD 350 %350 %ASTM D882
Film Elongation at Break, TD 790 %790 %ASTM D882
Elmendorf Tear Strength MD 90 g90 gASTM D1922
Elmendorf Tear Strength TD 350 g350 gASTM D1922
Dart Drop Test 180 g0.397 lbASTM D1709A
Film Tensile Strength at Break, MD 22.1 MPa3200 psiASTM D882
Film Tensile Strength at Break, TD 15.9 MPa2300 psiASTM D882
1% Secant Modulus, MD 55.8 MPa8100 psiASTM D882
1% Secant Modulus, TD 56.5 MPa8200 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Melting Point 81.0 °C178 °FExxon Method
Vicat Softening Point 57.2 °C135 °FASTM D882

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil Optema® TC-110 Cast Ethylene Methyl Acrylate
ExxonMobil Optema® TC-110 Blown Ethylene Methyl Acrylate
ExxonMobil Optema® TC-110 Molding Ethylene Methyl Acrylate
ExxonMobil Optema® TC-114 Blown Ethylene Methyl Acrylate
ExxonMobil OPTEMA™ TC 120 ExCo Ethylene Methyl Acrylate

PEXCEXa / 140963

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.