MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Graft Polymer GRAFTALEN™ MP-UHHD 00850 Melt Processable Ultra-High-Molecular-Weight-Polyethylene based on High Density Polyethylene
Categories: Polymer; Thermoplastic; Polyethylene (PE)

Material Notes: GRAFTALEN™ MP-UHHD is a high performance polymer alloy, consisting of ultra-high molecular weight polyethylene and high density polyethylene. Its main characteristics are very high impact strength, which remains high even at low temperatures, and great flexural properties.

Applications: GRAFTALEN™ MP-UHHD functions as a toughener

  • Improves mechanical characteristics
  • Increases abrasion resistance. Supplied as Granulate.

    Information provided by Graft Polymer LTD.

  • Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 0.945 g/cc
    @Temperature 21.0 °C
    0.0341 lb/in³
    @Temperature 69.8 °F
    ASTM D792
    Melt Flow <= 8.1 g/10 min
    @Load 5.00 kg,
    Temperature 230 °C
    <= 8.1 g/10 min
    @Load 11.0 lb,
    Temperature 446 °F
    ISO 1133
     
    Mechanical PropertiesMetricEnglishComments
    Hardness, Shore D 6060ASTM D2240
    Tensile Strength at Break 27.1 - 32.9 MPa3930 - 4770 psiExtrusion Molded, 10mm/min; ISO 527-2
    Tensile Strength, Yield 17.2 - 20.0 MPa2490 - 2900 psiExtrusion Molded, 10mm/min; ISO 527-2
    Elongation at Break 335 - 401 %335 - 401 %Extrusion Molded, 10mm/min; ISO 527-2
    Flexural Strength 25.3 - 25.9 MPa3670 - 3760 psiExtrusion Molded, 2mm/min; ISO 178
    Charpy Impact Unnotched NB
    @Temperature -40.0 °C
    NB
    @Temperature -40.0 °F
    Extrusion Molded, Sample: 1eA(4J); ISO 179
    Charpy Impact, Notched  1.00 J/cm²
    @Temperature -40.0 °C
    4.76 ft-lb/in²
    @Temperature -40.0 °F
    ISO 179
     NB
    @Temperature 23.0 °C
    NB
    @Temperature 73.4 °F
    Extrusion Molded, Sample: 1eA(4J); ISO 179
    Taber Abrasion, mg/1000 Cycles 3.6
    @Load 1.02 kg
    3.6
    @Load 2.25 lb
    at 72 rpm; ASTM D4060
     
    Thermal PropertiesMetricEnglishComments
    Vicat Softening Point 123 °C
    @Load 1.02 kg
    253 °F
    @Load 2.25 lb
    ISO 306
     
    Descriptive Properties
    Bend Stress (MPa)579 +- 110ISO 178. Extrusion Molded. @ 6mm sample thickness. 2mm/min
    Flexural Elongation (mm)5.7 +-0.2ISO 178. Extrusion Molded. @ max load. 2mm/min

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    PGRAFT934 / 232365

    Rulon Bearings

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.