MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

Special Metals INCONEL® G-3 Nickel Superalloy (UNS N06985)
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: A nickel-chromium-iron alloy with additions of molybdenum and copper. It has good weldability and resistance to intergranular corrosion in the welded condition. The low carbon content helps prevent sensitization and consequent intergranular corrosion of weld heat-affected zones. Used for flue-gas scrubbers and for handling phosphoric and sulfuric acids.

Data provided by the manufacturer, Special Metals.

Key Words: ASTM B 366, B 581, B 582, B 619, B 622, B 626, B 751, B 775, B 829
NACE MR-0175/ISO 15156
ASME SB-366, SB-581, SB-582, SB-619, SB-622, SB-626, SB-751, SB-775, SB-829
DIN 17744, 17750 – 17752
Werkstoff Nr. 2.4619
ISO 6207, 6208, 9724
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.30 g/cc0.300 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate >= 621 MPa>= 90000 psiMin per ASTM B582; Sheet and Plate
Tensile Strength, Yield >= 241 MPa
@Strain 0.2 %
>= 35000 psi
@Strain 0.2 %
Min per ASTM B582; Sheet and Plate
Elongation at Break >= 45 %>= 45 %Min per ASTM B582; Sheet and Plate
Tensile Modulus 199 GPa28900 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear  14.6 µm/m-°C
@Temperature 24.0 - 100 °C
8.11 µin/in-°F
@Temperature 75.2 - 212 °F
Mean
 14.6 µm/m-°C
@Temperature 24.0 - 300 °C
8.11 µin/in-°F
@Temperature 75.2 - 572 °F
Mean
 15.1 µm/m-°C
@Temperature 24.0 - 500 °C
8.39 µin/in-°F
@Temperature 75.2 - 932 °F
Mean
Specific Heat Capacity 0.453 J/g-°C0.108 BTU/lb-°F
Thermal Conductivity 10.0 W/m-K69.4 BTU-in/hr-ft²-°F
Melting Point 1260 - 1343 °C2300 - 2449 °F
Solidus 1260 °C2300 °F
Liquidus 1343 °C2449 °F
 
Component Elements PropertiesMetricEnglishComments
Chromium, Cr 21 - 23.5 %21 - 23.5 %
Copper, Cu 1.5 - 2.5 %1.5 - 2.5 %
Iron, Fe 18 - 21 %18 - 21 %
Molybdenum, Mo 6.0 - 8.0 %6.0 - 8.0 %
Nickel, Ni 49 %49 %As remainder

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Special Metals INCONEL® Alloy 718
Special Metals INCONEL® HX Nickel Superalloy (UNS N06002)
Special Metals INCONEL® Alloy 600
Special Metals INCONEL® Alloy 751
Special Metals INCONEL® Alloy X-750

NINCO09 / 17442

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.