Physical Properties | Metric | English | Comments |
---|
Density | 9.22 g/cc | 0.333 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength, Ultimate | 855 MPa | 124000 psi |
Modulus of Elasticity | 217 GPa | 31500 ksi |
| 117 GPa @Temperature 1000 °C | 17000 ksi @Temperature 1830 °F |
| 134 GPa @Temperature 900 °C | 19400 ksi @Temperature 1650 °F |
| 149 GPa @Temperature 800 °C | 21600 ksi @Temperature 1470 °F |
| 159 GPa @Temperature 700 °C | 23100 ksi @Temperature 1290 °F |
| 167 GPa @Temperature 600 °C | 24200 ksi @Temperature 1110 °F |
| 173 GPa @Temperature 500 °C | 25100 ksi @Temperature 932 °F |
| 179 GPa @Temperature 400 °C | 26000 ksi @Temperature 752 °F |
| 185 GPa @Temperature 300 °C | 26800 ksi @Temperature 572 °F |
| 191 GPa @Temperature 200 °C | 27700 ksi @Temperature 392 °F |
| 199 GPa @Temperature 100 °C | 28900 ksi @Temperature 212 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000137 ohm-cm @Temperature 0.000 °C | 0.000137 ohm-cm @Temperature 32.0 °F |
| 0.000138 ohm-cm @Temperature 100 °C | 0.000138 ohm-cm @Temperature 212 °F |
| 0.000138 ohm-cm @Temperature 200 °C | 0.000138 ohm-cm @Temperature 392 °F |
| 0.000139 ohm-cm @Temperature 300 °C | 0.000139 ohm-cm @Temperature 572 °F |
| 0.000139 ohm-cm @Temperature 400 °C | 0.000139 ohm-cm @Temperature 752 °F |
| 0.000141 ohm-cm @Temperature 500 °C | 0.000141 ohm-cm @Temperature 932 °F |
| 0.000146 ohm-cm @Temperature 600 °C | 0.000146 ohm-cm @Temperature 1110 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 10.3 µm/m-°C @Temperature 20.0 - 93.0 °C | 5.72 µin/in-°F @Temperature 68.0 - 199 °F |
| 10.8 µm/m-°C @Temperature 20.0 - 204 °C | 6.00 µin/in-°F @Temperature 68.0 - 399 °F |
| 11.2 µm/m-°C @Temperature 20.0 - 316 °C | 6.22 µin/in-°F @Temperature 68.0 - 601 °F |
| 11.5 µm/m-°C @Temperature 20.0 - 427 °C | 6.39 µin/in-°F @Temperature 68.0 - 801 °F |
| 11.7 µm/m-°C @Temperature 20.0 - 538 °C | 6.50 µin/in-°F @Temperature 68.0 - 1000 °F |
Specific Heat Capacity | 0.373 J/g-°C @Temperature 0.000 °C | 0.0891 BTU/lb-°F @Temperature 32.0 °F |
| 0.389 J/g-°C @Temperature 100 °C | 0.0930 BTU/lb-°F @Temperature 212 °F |
| 0.406 J/g-°C @Temperature 200 °C | 0.0970 BTU/lb-°F @Temperature 392 °F |
| 0.423 J/g-°C @Temperature 300 °C | 0.101 BTU/lb-°F @Temperature 572 °F |
| 0.431 J/g-°C @Temperature 400 °C | 0.103 BTU/lb-°F @Temperature 752 °F |
| 0.444 J/g-°C @Temperature 500 °C | 0.106 BTU/lb-°F @Temperature 932 °F |
| 0.456 J/g-°C @Temperature 600 °C | 0.109 BTU/lb-°F @Temperature 1110 °F |
Thermal Conductivity | 11.1 W/m-K @Temperature 0.000 °C | 77.0 BTU-in/hr-ft²-°F @Temperature 32.0 °F |
| 12.2 W/m-K @Temperature 100 °C | 84.7 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 13.4 W/m-K @Temperature 200 °C | 93.0 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 14.6 W/m-K @Temperature 300 °C | 101 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 16.0 W/m-K @Temperature 400 °C | 111 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 17.3 W/m-K @Temperature 500 °C | 120 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 18.7 W/m-K @Temperature 600 °C | 130 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | 0.010 % | 0.010 % |
Chromium, Cr | 1.0 % | 1.0 % |
Cobalt, Co | <= 1.0 % | <= 1.0 % |
Iron, Fe | <= 2.0 % | <= 2.0 % |
Manganese, Mn | <= 1.0 % | <= 1.0 % |
Molybdenum, Mo | 28 % | 28 % |
Nickel, Ni | 69 % | 69 % |
Silicon, Si | <= 0.10 % | <= 0.10 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.