MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

DuPont Elvax® 3173SHB Ethylene-Vinyl Acetate Copolymer Resin for Coextrusion, Blown Film  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate Copolymer (EVA), Extrusion/Coating Grade

Material Notes: 18 wt% Vinyl Acetate.

Elvax® 3173SHB is an extrudable ethylene-vinyl acetate copolymer resin available in pellet form for use in conventional extrusion equipment designed to process polyethylene resins.

Additives: Slip, Antiblock, Non-BHT antioxidant.

Applications: Elvax® 3173SHB is designed to provide a low-temperature heat seal to itself or many other materials commonly used in flexible packaging applications. The melt properties of this resin allow it to be processed on blown film equipment over a wide range of film thicknesses and blow-up ratios. It can also be coextruded with a variety of other polymers. Elvax® 3173SHB is typically used as a low-temperature seal layer in coextruded films.

Information provided by DuPont Packaging Polymers.

This product line/trade name was acquired by Dow, but this specific grade was discontinued prior to the acquisition.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.950 g/cc0.0343 lb/in³ASTM D792
Moisture Vapor Transmission 1.40 cc-mm/m²-24hr-atm3.56 cc-mil/100 in²-24hr-atmg-mm/m²-day; based on 1 mil (0.0254 mm) thick film; ASTM E96
Oxygen Transmission 220 cc-mm/m²-24hr-atm
@Thickness 0.0254 mm
559 cc-mil/100 in²-24hr-atm
@Thickness 0.00100 in
Based on 1 mil (0.0254 mm) thick film; ASTM D3985
Viscosity 1.00e+6 cP
@Shear Rate 50 1/s,
Temperature 190 °C
1.00e+6 cP
@Shear Rate 50 1/s,
Temperature 374 °F
estimated from log-log graph
Melt Flow 2.5 g/10 min2.5 g/10 minCondition not noted.; ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Elongation at Break, MD 550 %550 %50 µm (2 mil) film; ASTM D882
Film Elongation at Break, TD 600 %600 %50 µm (2 mil) film; ASTM D882
Secant Modulus, MD 0.0480 GPa6.96 ksi50 µm (2 mil) film; ASTM D882
Secant Modulus, TD 0.0440 GPa6.38 ksi50 µm (2 mil) film; ASTM D882
Impact 2828J/mm Spencer Impact; ASTM D3420
Coefficient of Friction 0.250.25film/film; ASTM D1894
 0.440.44film/metal; ASTM D1894
Elmendorf Tear Strength, MD 3.70 g/micron94.0 g/mil50 µm (2 mil) film; ASTM D1922
Elmendorf Tear Strength, TD 4.25 g/micron108 g/mil50 µm (2 mil) film; ASTM D1922
Film Tensile Strength at Break, MD 23.0 MPa3340 psi50 µm (2 mil) film; ASTM D882
Film Tensile Strength at Break, TD 28.0 MPa4060 psi50 µm (2 mil) film; ASTM D882
 
Thermal PropertiesMetricEnglishComments
Melting Point 65.0 °C149 °FFreezing Point via DSC/ASTM D3418
 87.0 °C189 °FUpon Melting via DSC/ASTM D3418
Vicat Softening Point 65.0 °C149 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Haze 15 %15 %ASTM D1003
Gloss 50 %50 %20°; ASTM D2457
Transmission, Visible 4.5 %4.5 %50 µm (2 mil) film; ASTM D1746

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Elvax® 3121A Ethylene-Vinyl Acetate Copolymer Resin for Blown Film
DuPont Elvax® 210 Ethylene Vinyl Acetate
DuPont Elvax® 205W Ethylene Vinyl Acetate
DuPont Elvax® 150W-LG Ethylene Vinyl Acetate
DuPont Elvax® 3128 Ethylene-Vinyl Acetate Copolymer Resin for Blown Film

PDUPHI / 33621

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.