MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Outokumpu 4565 High Performance Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Austenitic; Pressure Vessel Steel; Stainless Steel

Material Notes:

Applications:

  • Process equipment in chemical industry
  • Bleaching equipment in the pulp and paper industry
  • Flue-gas cleaning
  • Desalination
  • Seawater handling
  • Heat exchangers

Available in hot rolled plate (Quarto) form.

Key Words: EN 1.4565; UNS S34565
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.00 g/cc0.289 lb/in³RT
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell >= 240>= 240Hot rolled plate/Hot rolled strip/Cold rolled strip; EN 10003-1
Tensile Strength, Ultimate 825 MPa120000 psiOutokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 610 MPa
@Temperature 400 °C
88500 psi
@Temperature 752 °F
EN min.; EN 10002-5
 640 MPa
@Temperature 200 °C
92800 psi
@Temperature 392 °F
EN min.; EN 10002-5
 640 MPa
@Temperature 300 °C
92800 psi
@Temperature 572 °F
EN min.; EN 10002-5
 750 MPa
@Temperature 100 °C
109000 psi
@Temperature 212 °F
EN min.; EN 10002-5
Tensile Strength, Yield  420 MPa
@Strain 0.2 %
60900 psi
@Strain 0.2 %
EN min., RT; EN 10002-1
 440 MPa
@Strain 0.2 %
63800 psi
@Strain 0.2 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 480 MPa
@Strain 1 %
69600 psi
@Strain 1 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 210 MPa
@Strain 0.2 %,
Temperature 400 °C
30500 psi
@Strain 0.2 %,
Temperature 752 °F
EN min.; EN 10002-5
 240 MPa
@Strain 0.2 %,
Temperature 300 °C
34800 psi
@Strain 0.2 %,
Temperature 572 °F
EN min.; EN 10002-5
 240 MPa
@Strain 1 %,
Temperature 400 °C
34800 psi
@Strain 1 %,
Temperature 752 °F
EN min.; EN 10002-5
 270 MPa
@Strain 1 %,
Temperature 300 °C
39200 psi
@Strain 1 %,
Temperature 572 °F
EN min.; EN 10002-5
 270 MPa
@Strain 0.2 %,
Temperature 200 °C
39200 psi
@Strain 0.2 %,
Temperature 392 °F
EN min.; EN 10002-5
 310 MPa
@Strain 1 %,
Temperature 200 °C
45000 psi
@Strain 1 %,
Temperature 392 °F
EN min.; EN 10002-5
 350 MPa
@Strain 0.2 %,
Temperature 100 °C
50800 psi
@Strain 0.2 %,
Temperature 212 °F
EN min.; EN 10002-5
 400 MPa
@Strain 1 %,
Temperature 100 °C
58000 psi
@Strain 1 %,
Temperature 212 °F
EN min.; EN 10002-5
Elongation at Break 55 %55 %Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
Modulus of Elasticity 190 GPa27600 ksiRT
 165 GPa
@Temperature 400 °C
23900 ksi
@Temperature 752 °F
Impact Test >= 90.0 J>= 66.4 ft-lbHot rolled plate/Hot rolled strip/Cold rolled strip; EN 10045-1
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000920 ohm-cm0.0000920 ohm-cmRT
 
Thermal PropertiesMetricEnglishComments
CTE, linear  14.5 µm/m-°C
@Temperature 100 °C
8.06 µin/in-°F
@Temperature 212 °F
 16.8 µm/m-°C
@Temperature 400 °C
9.33 µin/in-°F
@Temperature 752 °F
Specific Heat Capacity 0.450 J/g-°C0.108 BTU/lb-°FRT
Thermal Conductivity 12.0 W/m-K83.3 BTU-in/hr-ft²-°FRT
 18.0 W/m-K
@Temperature 400 °C
125 BTU-in/hr-ft²-°F
@Temperature 752 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 1120 - 1170 °C2050 - 2140 °FSolution Annealing
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.020 %0.020 %
Chromium, Cr 24 %24 %
Iron, Fe 48.53 %48.53 %
Manganese, Mn 5.5 %5.5 %
Molybdenum, Mo 4.5 %4.5 %
Nickel, Ni 17 %17 %
Nitrogen, N 0.45 %0.45 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Outokumpu 254 SMO® High Performance Austenitic Stainless Steel
Outokumpu 904L High Performance Austenitic Stainless Steel
ASTM A516, Grade 60
ASTM A285, Grade A
ASTM A285, Grade C

NOUTOK35 / 18750

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.