MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

NOVA Chemicals SURPASS® FPs117-D Octene Copolymer sLLDPE Film Resin
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade; LLDPE/Octene, Film

Material Notes: Features: easy processability, superior toughness with excellent tear strength, excellent seal properties, low gel. Common additives: processing antioxidant, polymer process aid, slip (1000 ppm), AB (2500 ppm), PPA.

Applications: Lamination film, co-extruded sealant layer, and high toughness film.

Film properties reported are typical of blown film extruded on a 2.5" extruder with 4" die and 35-mil die gap at a blow up ratio of 2.5:1, but are dependent upon operating conditions.

Information provided by NOVA Chemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.917 g/cc0.0331 lb/in³ASTM D 792
Thickness 25.0 microns0.984 milAs tested
Melt Index of Compound 1.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
1.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D 1238
Antiblock Level 2500 ppm2500 ppm
Slip Level 1000 ppm1000 ppm
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 9.00 MPa1310 psiASTM D882
Film Tensile Strength at Yield, TD 9.00 MPa1310 psiASTM D882
Film Elongation at Break, MD 540 %540 %ASTM D882
Film Elongation at Break, TD 760 %760 %ASTM D882
Elmendorf Tear Strength MD 300 g
@Thickness 0.0250 mm
300 g
@Thickness 0.000984 in
ASTM D1922
Elmendorf Tear Strength TD 450 g
@Thickness 0.0250 mm
450 g
@Thickness 0.000984 in
ASTM D1922
Dart Drop Test 400 g
@Thickness 0.0250 mm
0.882 lb
@Thickness 0.000984 in
F50; ASTM D1709/A
Film Tensile Strength at Break, MD 46.0 MPa6670 psiASTM D882
Film Tensile Strength at Break, TD 42.0 MPa6090 psiASTM D882
1% Secant Modulus, MD 126 MPa18300 psiASTM D882
1% Secant Modulus, TD 132 MPa19100 psiASTM D882
Heat Seal Strength Initiation Temperature 100 °C212 °FNOVA Chemicals test method
 
Optical PropertiesMetricEnglishComments
Haze  7.0 %
@Thickness 0.0250 mm
7.0 %
@Thickness 0.000984 in
LDPE blended; ASTM D1003
 16 %
@Thickness 0.0250 mm
16 %
@Thickness 0.000984 in
100% LLDPE; ASTM D1003
Gloss  37 %
@Thickness 0.0250 mm
37 %
@Thickness 0.000984 in
100% LLDPE, @ 45°; ASTM D2457
 72 %
@Thickness 0.0250 mm
72 %
@Thickness 0.000984 in
LDPE blended, @ 45°; ASTM D2457
 
Descriptive Properties
Low Friction Puncture79 J/mmNOVA Chemicals test

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PNOV605 / 249052

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.