MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 1060-O
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 1000 Series Aluminum

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
The aluminum content for unalloyed aluminum not made by a refining process is the difference between 100.00 percent and the sum of all other analyzed metallic elements present in amounts of 0.010 percent of more each, expressed to the second decimal before determining the sum. For alloys and unalloyed aluminum not made by a refining process, when the specified maximum limit is 0.XX, an observed value or a calculated value greater than 0.005 but less than 0.010% is rounded off and shown as " less than 0.01%".
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 1060-O; UNS A91060; AA1060-O; Al1060-O
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.705 g/cc0.09772 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 1919AA; Typical; 500 g load; 10 mm ball
Tensile Strength, Ultimate 68.9 MPa10000 psiAA; Typical
 55.0 - 95.0 MPa7980 - 13800 psiSheet and plate
 >= 58.0 MPa
@Thickness 0.254 - 12.7 mm
>= 8410 psi
@Thickness 0.0100 - 0.500 in
Drawn tube
 58.0 - 95.0 MPa
@Thickness 1.27 - 4.29 mm
8410 - 13800 psi
@Thickness 0.0500 - 0.169 in
Extruded tube
Tensile Strength, Yield >= 17.0 MPa>= 2470 psiSheet and plate
 >= 17.0 MPa>= 2470 psiExtruded tube
 27.6 MPa4000 psiAA; Typical
 >= 17.0 MPa
@Thickness 0.254 - 12.7 mm
>= 2470 psi
@Thickness 0.0100 - 0.500 in
Drawn tube
Elongation at Break 15 - 25 %15 - 25 %Sheet and plate
 43 %
@Thickness 1.59 mm
43 %
@Thickness 0.0625 in
AA; Typical
Modulus of Elasticity 68.9 GPa10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Ultimate Bearing Strength 117 MPa17000 psiEdge distance/pin diameter = 2.0
Bearing Yield Strength 41.0 MPa5950 psiEdge distance/pin diameter = 2.0
Poissons Ratio 0.330.33
Fatigue Strength 20.7 MPa
@# of Cycles 5.00e+8
3000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Machinability 10 %10 %0-100 Scale of Aluminum Alloys
Shear Modulus 26.0 GPa3770 ksiCalculated
Shear Strength 48.3 MPa7000 psiAA; Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000283 ohm-cm
@Temperature 20.0 °C
0.00000283 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 390 J/g168 BTU/lb
CTE, linear  21.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
12.1 µin/in-°F
@Temperature -58.0 - 68.0 °F
 23.6 µm/m-°C
@Temperature 20.0 - 100 °C
13.1 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 24.5 µm/m-°C
@Temperature 20.0 - 200 °C
13.6 µin/in-°F
@Temperature 68.0 - 392 °F
 25.5 µm/m-°C
@Temperature 20.0 - 300 °C
14.2 µin/in-°F
@Temperature 68.0 - 572 °F
 25.5 µm/m-°C
@Temperature 20.0 - 300 °C
14.2 µin/in-°F
@Temperature 68.0 - 572 °F
average
Specific Heat Capacity 0.900 J/g-°C0.215 BTU/lb-°F
Thermal Conductivity 234.2 W/m-K1625 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 646.1 - 657.2 °C1195 - 1215 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 646.1 °C1195 °FAA; Typical
Liquidus 657.2 °C1215 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 343 °C650 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al >= 99.60 %>= 99.60 %Specified
Copper, Cu <= 0.05 %<= 0.05 %
Iron, Fe <= 0.35 %<= 0.35 %
Magnesium, Mg <= 0.03 %<= 0.03 %
Manganese, Mn <= 0.03 %<= 0.03 %
Other, each <= 0.03 %<= 0.03 %
Silicon, Si <= 0.25 %<= 0.25 %
Titanium, Ti <= 0.03 %<= 0.03 %
Vanadium, V <= 0.05 %<= 0.05 %
Zinc, Zn <= 0.05 %<= 0.05 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 1100-O
Aluminum 1060-H12
Aluminum 1060-H18
Aluminum 1050-O
Aluminum 1060-H14

MA1060O / 8732

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.