Vanadium Carbide, VC
Categories: Ceramic; Carbide

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 5.71 g/cc0.206 lb/in³theoretical
Molecular Weight 62.953 g/mol62.953 g/mol
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell A 9191at RT
Vickers Microhardness 29502950
Modulus of Elasticity 268 - 420 GPa38900 - 60900 ksiat RT
Compressive Strength 607 MPa88000 psiat RT
Poissons Ratio 0.220.22at RT
Shear Modulus 157 GPa22800 ksiat RT
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000150 ohm-cm0.000150 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 7.20 µm/m-°C
@Temperature 20.0 °C
4.00 µin/in-°F
@Temperature 68.0 °F
Melting Point 2730 °C4950 °F
Solidus 2655 °C4811 °F
Liquidus 2810 °C5090 °F
 
Descriptive Properties
ColorBlack
Crystal StructureCubicNaCl Structure

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.