MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Wolf Kunststoff ZEDEX® ZX-530EL3 066 Polymer Alloy, Carbon Fiber Reinforced
Categories: Polymer; Thermoplastic

Material Notes: Main Characteristics: Low thermal expansion; High rigidity; High yield stress; High wear resistance; Low friction; Stress Resistant
Applications: Chemical Engineering; Laboratory Technology; Automitve Technology; Machine Tools

Information provided by Zedex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.30 g/ccISO 1183
Water Absorption 0.010 %
@Temperature 23.0 °C
RMC 93%; DIN EN ISO 62
Moisture Absorption at Equilibrium 0.050 %DIN EN ISO 62
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A >= 100DIN 53505
Hardness, Shore D 81DIN 53505
Ball Indentation Hardness 107 MPaDIN 2039
Tensile Strength at Break 50.0 MPaDIN EN ISO 527
Tensile Strength 50.0 MPaDIN EN ISO 527
Tensile Strength, Yield 38.0 MPaElastic Limit
Tensile Stress at Strain 14.0 MPa
@Strain 1 %,
Time 3.60e+6 sec
DIN 53444
Elongation at Break 20 %DIN EN ISO 527
Elongation at Yield 3.4 %Elastic Yield Point
 20 %Elongation at Maximum Force; DIN EN ISO 527
Tensile Modulus 1500 MPaDIN EN ISO 527
Flexural Strength 63.0 MPaOuter Fiber Stress at 3.5% Outer Fiber Strain; DIN EN ISO 178
 70.0 MPaDIN EN ISO 178
Flexural Modulus 2320 MPaDIN EN ISO 178
Flexural Strain at Yield 5.6 %DIN EN ISO 178
Compressive Strain at Break 30 %Nominal Compressive Strain at Compressive Strength; DIN EN ISO 604
Compressive Strain at Yield 7.2 %Nominal; DIN EN ISO 604
Compressive Yield Strength 50.4 MPaElastic Limit
Compressive Strength 19.0 MPa
@Time 3.60e+7 sec
 43.0 MPa
@Time 360000 sec
 54.0 MPa
@Time 36.0 sec
 40.5 MPa
@Strain 3.5 %
DIN EN ISO 604
Compressive Modulus 1750 MPaDIN EN ISO 604
Fatigue Strength 6.00 MPa
@# of Cycles 1.00e+6
1 Hz
K Factor (ISO) 0.30 µm/km
@Temperature 20.0 °C
 1.0 µm/km
@Temperature 100 °C
Charpy Impact Unnotched 23.5 kJ/m²EN ISO 179/1eU
Charpy Impact, Notched NBEN ISO 179/1eA
Coefficient of Friction, Dynamic 0.080
@Temperature 100 °C
Dry Operation
 0.13
@Temperature 20.0 °C
Dry Operation
Coefficient of Friction, Static 0.21
@Temperature 20.0 °C
Dry Operation
Tensile Creep Modulus, 1000 hours 1300 MPaAt 1% Deformation; DIN 53444
Limiting Pressure Velocity 0.1500 MPa-m/secv = 200m/min
 0.167 MPa-m/secv = 100m/min
 0.356 MPa-m/secv = 1m/min
 0.967 MPa-m/secv = 10m/min
Compression Set 5.0 %Elastic Compression Limit
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+13 ohm-cmIEC 93
Surface Resistance 6.50e+12 ohmIEC 93
Dielectric Constant 4.1
@Frequency 110 Hz
IEC 250
Dielectric Strength 21.5 kV/mmIEC 243
Dissipation Factor 0.030
@Frequency 110 Hz
IEC 112
Comparative Tracking Index 130 VIEC 112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 60.0 µm/m-°C
@Temperature <=100 °C
ISO E 830
 67.0 µm/m-°C
@Temperature <=150 °C
ISO E 831
Specific Heat Capacity 1.81 J/g-°CDSC
Melting Point 320 °CDSC
Maximum Service Temperature, Air 70.0 °CPressed Bushings
 240 °CContinuous
 260 °CShort Term (3h)
Deflection Temperature at 1.8 MPa (264 psi) 117 °CDIN EN ISO 75
Glass Transition Temp, Tg 90.0 °CDSC
 
Descriptive Properties
Alignment Adjustment2Nominal Scale: 1, low; 10, high
Chemical Sterilization10Nominal Scale: 1, low; 10, high
ColorBeige
Creep Resistance7Nominal Scale: 1, low; 10, high
Dimensional Stability with Thermal Expansion7Nominal Scale: 1, low; 10, high
Free from SiliconApplicable
Gamma-rays Radiation Sterilization4Nominal Scale: 1, low; 10, high
Injection Molded PartsApplicable
Machined PartsApplicable
Moist Heat Sterilization6Nominal Scale: 1, low; 10, high
Plastic GranulesApplicable
Rate of Desorption3.12E-07a = .49
Resistance Against dust, Dirt, Abrasive Substances6Nominal Scale: 1, low; 10, high
Resistance Against Hot Water140
Resistance to Chemicals9Nominal Scale: 1, low; 10, high
Resistant Against DisinfectantApplicable
Rods up to Øe (de)Applicable
Sheets up to Maximum ThicknessApplicable
Sliding Velocity100
Suitable for Outdoor Use7Nominal Scale: 1, low; 10, high
Suitable for Use in WaterApplicable
Suitable for VacuumApplicable
Tubes (hollow rods) up to Øe (de)Applicable
UV Rays Resistance8Nominal Scale: 1, low; 10, high
UV-Sterilization7Nominal Scale: 1, low; 10, high

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Wolf Kunststoff ZEDEX® ZX-324V1T A3H PEEK Polymer, Reinforced
Wolf Kunststoff ZEDEX® ZX-324VMT A3B PEEK, Fiber Reinforced
Lehvoss LUVOCOM® 1105-8000 PEEK with carbon fiber, lubricant modified
CRP Technology AMC225xe Aluminum Alloy - SiC Composite, T4 Condition
Overview of materials for Polyimide

PZEDEX14 / 122129

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.