MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Pressure Seal 19748 Silicone
Categories: Polymer; Thermoset; Silicone

Material Notes: Compound 19748 is a 70 durometer salmon colored Silicone elastomer, it is formulated with FDA sanctioned materials. It exhibits good resistance to heat and will remain non brittle at very low temperatures. This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 5 GE 709 A19 B37 EA14 EO16 EO36 F19 G11; 6 GE 709 A19 B37 EA14 EO16 EO36 F19 G11; 7 GE 709 A19 B37 EA14 EO16 EO36 F19 G11; 3 FC 710 A19 B37 EA14 EO16 F1-11 G11; M5 GE 706 A19 B37 EA14 EO16 EO36 F19 G11
ZZ-R-765 Class 2a & 2b Grade 70
A-A-59588 Class 2a & 2b Grade 70
3-A Sanitary Standards 18-03 Class III & IV
AMS 3304
CFR 21 177.2600
This Compound is RoHS Compliant

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.19 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 72
 55
@Temperature 150 °C,
Time 252000 sec
ASTM OIL #3 (IRM 903)
 68
@Temperature 175 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 69
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 72
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 74
@Temperature 200 °C,
Time 252000 sec
Heat Aged
 76
@Temperature 225 °C,
Time 252000 sec
Heat Aged
Tensile Strength 1032 psi
 909.2 psi
@Temperature 175 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 985.6 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 1077.4 psi
@Temperature 225 °C,
Time 252000 sec
Heat Aged
 1281.7 psi
@Temperature 200 °C,
Time 252000 sec
Heat Aged
Elongation, Ultimate 247 %
 231.9 %
@Temperature 175 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 238.1 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 243 %
@Temperature 225 °C,
Time 252000 sec
Heat Aged
 289 %
@Temperature 200 °C,
Time 252000 sec
Heat Aged
100% Modulus 397 psi
Tear Strength 72.0 pliDie B
 90.0 pliDie C
Compression Set 11.5 %
@Temperature 175 °C,
Time 79200 sec
Plied
 13.9 %
@Temperature 150 °C,
Time 252000 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature <= -123 °F
Shrinkage 0.00 %
@Temperature 100 °C,
Time 252000 sec
Volume, Distilled water aged
 3.8 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 5.4 %
@Temperature 175 °C,
Time 252000 sec
Volume, ASTM Oil #1
 42.8 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #3
 
Descriptive Properties
ColorSalmon
TR-10 Temperature-45°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL171 / 318381

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.