System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
SABIC VALOX™ 4031 PBT (Europe)
Categories:
Polymer
;
Thermoplastic
;
Polyester, TP
;
Polybutylene Terephthalate (PBT)
Material Notes:
VALOX 4031 is a 30% high strength glass fibre reinforced PBT injection moulding resin with excellent strength, stiffness and heat resistance. Applications: appliance handles, spotlights, electric motors.
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Specific Gravity
1.54
g/cc
ASTM D792
Density
1.54
g/cc
ISO 1183
Filler Content
30 %
ASTM D229
Water Absorption
0.26 %
23°C/sat; ISO 62
Moisture Absorption
0.0600 %
23°C / 50% RH; ISO 62
Viscosity
150
cP
@Shear Rate 1500 1/s,
Temperature 260 °C
melt; ISO 11443
Linear Mold Shrinkage, Flow
0.0030
-
0.0070
cm/cm
SABIC method
Linear Mold Shrinkage, Transverse
0.0050
-
0.010
cm/cm
SABIC method
Melt Flow
12
g/10 min
@Load 2.16 kg,
Temperature 250 °C
cm³/10 min; ISO 1133
30
g/10 min
@Load 5.00 kg,
Temperature 250 °C
cm³/10 min; ISO 1133
40
g/10 min
@Load 5.00 kg,
Temperature 265 °C
cm³/10 min; ISO 1133
50
g/10 min
@Load 5.00 kg,
Temperature 266 °C
ASTM D1238
Mechanical Properties
Original Value
Comments
Hardness, Rockwell R
125
ISO 2039-2
Ball Indentation Hardness
125
MPa
ISO 2039-1
Tensile Strength at Break
135
MPa
5 mm/min; ISO 527
140
MPa
5 mm/min; ASTM D638
Tensile Strength, Yield
135
MPa
5 mm/min; ISO 527
140
MPa
5 mm/min; ASTM D638
Elongation at Break
2.0 %
5 mm/min; ISO 527
3.0 %
5 mm/min; ASTM D638
Elongation at Yield
2.0 %
5 mm/min; ISO 527
3.0 %
5 mm/min; ASTM D638
Tensile Modulus
10000
MPa
5 mm/min; ASTM D638
10000
MPa
1mm/min; ISO 527
Flexural Strength
190
MPa
brk, 1.3 mm/min, 50 mm span; ASTM D790
200
MPa
2 mm/min; break; ISO 178
Flexural Yield Strength
190
MPa
1.3 mm/min, 50 mm span; ASTM D790
210
MPa
2 mm/min; ISO 178
Flexural Modulus
7900
MPa
1.3 mm/min, 50 mm span; ASTM D790
8300
MPa
2 mm/min; ISO 178
Flexural Strain at Break
3.0 %
2 mm/min; ISO 178
Izod Impact, Notched
100
J/m
ASTM D256
100
J/m
@Temperature -30.0 °C
ASTM D256
100
J/m
@Temperature 0.000 °C
ASTM D256
Izod Impact, Unnotched
880
J/m
ASTM D4812
880
J/m
@Temperature -30.0 °C
ASTM D4812
Izod Impact, Notched (ISO)
11.0
kJ/m²
80*10*4; ISO 180/1A
10.0
kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
11.0
kJ/m²
@Temperature 0.000 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO)
55.0
kJ/m²
80*10*4; ISO 180/1U
55.0
kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1U
Charpy Impact Unnotched
50.0
kJ/m²
Edgew 80*10*4 sp=62mm; ISO 179/1eU
65.0
kJ/m²
ISO 179/2C
55.0
kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eU
60.0
kJ/m²
@Temperature -30.0 °C
ISO 179/2C
Charpy Impact, Notched
7.00
kJ/m²
Edgew 80*10*4 sp=62mm; ISO 179/1eA
12.0
kJ/m²
ISO 179/2C
6.00
kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
12.0
kJ/m²
@Temperature -30.0 °C
ISO 179/2C
Electrical Properties
Original Value
Comments
Volume Resistivity
>=
1.00e+15
ohm-cm
IEC 60093
>=
1.00e+15
ohm-cm
ASTM D257
Surface Resistance
>=
1.00e+15
ohm
ROA; IEC 60093
Dielectric Constant
3.1
@Frequency 1e+6 Hz
IEC 60250
3.3
@Frequency 50.0 - 60.0 Hz
IEC 60250
Dielectric Strength
15.0
kV/mm
@Thickness 3.20 mm
in oil; IEC 60243-1
18.0
kV/mm
@Thickness 3.20 mm
in oil; ASTM D149
24.0
kV/mm
@Thickness 1.60 mm
in oil; ASTM D149
24.0
kV/mm
@Thickness 1.60 mm
in oil; IEC 60243-1
26.0
kV/mm
@Thickness 0.800 mm
in oil; IEC 60243-1
26.0
kV/mm
@Thickness 0.800 mm
in oil; ASTM D149
Dissipation Factor
0.0016
@Frequency 50.0 - 60.0 Hz
IEC 60250
0.014
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance
120
-
180
sec
ASTM D495
Comparative Tracking Index
250
V
IEC 60112
>=
600
V
UL 746A
Hot Wire Ignition, HWI
60
-
120
sec
UL 746A
High Amp Arc Ignition, HAI
60
-
120
arcs
UL 746A
High Voltage Arc-Tracking Rate, HVTR
10.0
-
25.4
mm/min
UL 746A
Thermal Properties
Original Value
Comments
CTE, linear, Parallel to Flow
19.8
µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
21.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
30.0
µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow
74.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
120
µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
173
µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
Hot Ball Pressure Test
125
°C
IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi)
220
°C
Flatw 80*10*4 sp=64mm; ISO 75/Bf
220
°C
Edgew 120*10*4 sp=100mm; ISO 75/Be
220
°C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
205
°C
Flatw 80*10*4 sp=64mm; ISO 75/Af
210
°C
1.8 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
205
°C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point
215
°C
Rate B/50; ISO 306
215
°C
Rate B/50; ASTM D1525
215
°C
Rate B/120; ISO 306
220
°C
Rate A/50; ASTM D1525
220
°C
Rate A/50; ISO 306
UL RTI, Electrical
140
°C
UL 746B
UL RTI, Mechanical with Impact
140
°C
UL 746B
UL RTI, Mechanical without Impact
140
°C
UL 746B
Flammability, UL94
HB
@Thickness 0.840 mm
UL 94
HB
@Thickness 6.00 mm
UL 94
Glow Wire Test
750
°C
@Thickness 1.00 mm
IEC 60695-2-12
Processing Properties
Original Value
Comments
Processing Temperature
40.0
-
60.0
°C
Hopper Temperature
Nozzle Temperature
240
-
260
°C
Injection Molding
Zone 1
230
-
245
°C
Zone 2
240
-
255
°C
Zone 3
245
-
265
°C
Melt Temperature
250
-
270
°C
Mold Temperature
40.0
-
100
°C
Drying Temperature
110
-
120
°C
Injection Molding
Dry Time
2.00
-
4.00
hour
Injection Molding
Moisture Content
0.020 %
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
PSABI10250 / 243717
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.