MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Envalior Pocan® BFN 4231 000000 PBT, 25% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Glass Fiber Filled, Flame Retardant

Material Notes: PBT 25% glass fiber, general purpose, halogen free, flame retardant

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.52 g/ccISO 1183
Filler Content 25 %Glass Fiber
Linear Mold Shrinkage, Flow 0.0050 cm/cmPlaque 60 x 60 x 2mm; ISO 294-4
Linear Mold Shrinkage, Transverse 0.012 cm/cmPlaque 60 x 60 x 2mm; ISO 294-4
Melt Flow 40 g/10 min
@Load 5.00 kg,
Temperature 260 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 100 MPa5 mm/min; ISO 527-1,-2
Elongation at Break 2.2 %5 mm/min; ISO 527-1,-2
Tensile Modulus 10500 MPa1 mm/min; ISO 527-1,-2
Flexural Strain at Yield 2.4 %2 mm/min; ISO 178-A
Izod Impact, Unnotched (ISO) 33.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1U
 36.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1U
Charpy Impact Unnotched 35.0 kJ/m²
@Temperature -30.0 °C
ISO 179-1eU
 40.0 kJ/m²
@Temperature 23.0 °C
ISO 179-1eU
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 2.30e+14 ohm-cmIEC 60093
Surface Resistance 2.00e+16 ohmIEC 60093
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 30.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
CTE, linear, Transverse to Flow 90.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
Melting Point 220 °C10°C/min; ISO 11357-1,-3
Deflection Temperature at 0.46 MPa (66 psi) 210 °CMethod Af; ISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 224 °CMethod Bf; ISO 75-1,-2
Flammability, UL94 V-0
@Thickness 0.400 mm
UL Yellow Card
 5VA
@Thickness 1.50 mm
UL Yellow Card, NC, BK
Glow Wire Ignition Temperature 775 °C
@Thickness 0.750 mm
IEC 60695-2-13
 850 °C
@Thickness 0.400 mm
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 0.400 - 3.00 mm
IEC 60695-2-12
Shrinkage, MD 0.10 %
@Treatment Temp. 120 °C,
Time 14400 sec
Flow Direction Post-Molding, Plaque 60 x 60 x 2mm; ISO 294-4
Shrinkage, TD 0.10 %
@Treatment Temp. 120 °C,
Time 14400 sec
Post-Molding, Plaque 60 x 60 x 2mm; ISO 294-4
 
Processing PropertiesOriginal ValueComments
Melt Temperature 260 °CPlaque 60 x 60 x 2mm
Mold Temperature 80.0 °CPlaque 60 x 60 x 2mm
Hold Pressure 60.0 MPaPlaque 60 x 60 x 2mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Pocan® BFN 4211 000000 PBT, 13% Glass Fiber Reinforced
DuPont Mobility and Materials Crastin® FR684NH NC010 PBT-GF25FR(40)
DuPont Mobility and Materials Crastin® FR684NH BK591 PBT-GF25FR(40)

PLANW9058 / 208430

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.