MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Constellium Alumold® 500 Rolled Aluminum
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 5000 Series Aluminum Alloy

Material Notes: The Alumold® 500 alloy has been optimized to provide excellent machinability, good shape stability and high strength properties throughout the plate thickness. Uniform strength is an important property for mould and tool construction. Typical applications include compression or injection moulds for plastics.

Information provided by manufacturer

Key Words: IS 5615
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.82 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 175
@Thickness 203.2 - 254 mm
 175
@Thickness 254 - 305 mm
 180
@Thickness 127 - 152.4 mm
 180
@Thickness 152.4 - 203.2 mm
 185
@Thickness 25.0 - 76.2 mm
 185
@Thickness 76.2 - 127 mm
Tensile Strength >= 470 MPa
@Thickness 254 - 305 mm
Tempers T651 / T652
 >= 505 MPa
@Thickness 203.2 - 254 mm
Tempers T651 / T652
 510 MPa
@Thickness 254 - 305 mm
Typical Strength
 >= 525 MPa
@Thickness 152.4 - 203.2 mm
Tempers T651 / T652
 535 MPa
@Thickness 203.2 - 254 mm
Typical Strength
 >= 540 MPa
@Thickness 127 - 152.4 mm
Tempers T651 / T652
 >= 550 MPa
@Thickness 76.2 - 127 mm
Tempers T651 / T652
 555 MPa
@Thickness 152.4 - 203.2 mm
Typical Strength
 >= 560 MPa
@Thickness 25.0 - 76.2 mm
Tempers T651 / T652
 570 MPa
@Thickness 127 - 152.4 mm
Typical Strength
 580 MPa
@Thickness 76.2 - 127 mm
Typical Strength
 590 MPa
@Thickness 25.0 - 76.2 mm
Typical Strength
Tensile Strength, Yield >= 435 MPa
@Strain 0.2 %,
Thickness 254 - 305 mm
Tempers T651 / T652
 >= 455 MPa
@Strain 0.2 %,
Thickness 203.2 - 254 mm
Tempers T651 / T652
 470 MPa
@Strain 0.2 %,
Thickness 254 - 305 mm
Typical Strength
 >= 472 MPa
@Strain 0.2 %,
Thickness 127 - 152.4 mm
Tempers T651 / T652
 >= 473 MPa
@Strain 0.2 %,
Thickness 152.4 - 203.2 mm
Tempers T651 / T652
 490 MPa
@Strain 0.2 %,
Thickness 203.2 - 254 mm
Typical Strength
 >= 497 MPa
@Strain 0.2 %,
Thickness 76.2 - 127 mm
Tempers T651 / T652
 >= 504 MPa
@Strain 0.2 %,
Thickness 25.0 - 76.2 mm
Tempers T651 / T652
 510 MPa
@Strain 0.2 %,
Thickness 152.4 - 203.2 mm
Typical Strength
 520 MPa
@Strain 0.2 %,
Thickness 127 - 152.4 mm
Typical Strength
 530 MPa
@Strain 0.2 %,
Thickness 76.2 - 127 mm
Typical Strength
 540 MPa
@Strain 0.2 %,
Thickness 25.0 - 76.2 mm
Typical Strength
Elongation at Break >= 0.50 %
@Thickness 254 - 305 mm
Tempers T651 / T652
 >= 1.0 %
@Thickness 152.4 - 203.2 mm
Tempers T651 / T652
 >= 1.0 %
@Thickness 203.2 - 254 mm
Tempers T651 / T652
 1.5 %
@Thickness 203.2 - 254 mm
Typical Elongation
 1.5 %
@Thickness 254 - 305 mm
Typical Elongation
 2.0 %
@Thickness 152.4 - 203.2 mm
Typical Elongation
 >= 2.5 %
@Thickness 127 - 152.4 mm
Tempers T651 / T652
 >= 4.0 %
@Thickness 76.2 - 127 mm
Tempers T651 / T652
 4.0 %
@Thickness 127 - 152.4 mm
Typical Elongation
 >= 5.0 %
@Thickness 25.0 - 76.2 mm
Tempers T651 / T652
 6.0 %
@Thickness 76.2 - 127 mm
Typical Elongation
 10 %
@Thickness 25.0 - 76.2 mm
Typical Elongation
Modulus of Elasticity 73.0 GPacompression
Tensile Modulus 72.0 GPa
Poissons Ratio 0.33
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.7 µm/m-°C
@Temperature 20.0 - 100 °C
Specific Heat Capacity 0.857 J/g-°C
Thermal Conductivity 153 W/m-K
 
Descriptive Properties
Thermal Diffusivity63 mm²/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Constellium Alumold® 500 Forged Aluminum
RSP Technology RSA-7034 T6 Aluminum Super Alloy
Aluminum 7175-T66
Clinton Aluminum Alumold® 1-500 Forged
AISI E4340 Steel, annealed 810°C

NCONS014 / 160277

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.