MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
General Plastics LAST-A-FOAM® FR-4615 Foam
Categories: Other Engineering Material

Material Notes: Product Description: The LAST-A-FOAM®FR-4600 Microcell Series supports the most intricate detail while eliminating extra prep work. With an even-smoother surface finish than our LAST-A-FOAM® FR-4500 material, they are superb for prototypes and models, and precision tooling applications. Advanced microcell technology creates a grain-free, ultra smooth exterior for painted finishes, significantly reducing process time. What’s more, its finer cell structure is comparable to higher-density foam products without the added cost and weight.

Key Performance Benefits:

  • Ultra smooth finish
  • Lighter, less abrasive than syntactic boards
  • Creates intricate, 3-D details
  • Dimensionally stable
  • Special formulation allows creation of shavings when material is machined
  • Reduced cutting tool abrasion
  • Large sheets up to 60” x 120”
Applications:
  • 3-D Signage
  • Design prototypes
  • Appearance or “sight” models
  • Architectural models
  • Topographical maps
  • Tooling and molds for low temperature curing prepregs (<200ºF)
  • Decorative moldings

Information provided by General Plastics Manufacturing Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.240 g/ccASTM D1622
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 22ASTM D2240
Tensile Strength 460 psiPerpendicular to Rise; ASTM D1623
Flexural Strength 716 psiASTM D790
 930 psiRise Parallel to Beam Thick.; ASTM D790
 944 psiRise Parallel to Test Span; ASTM D790
Flexural Modulus 22749 psiASTM D790
 22749 psiRise Parallel to Beam Thick.; ASTM D790 Method 1-A
 25236 psiRise Parallel to Test Span; ASTM D790 Method 1-A
Compressive Strength 325 psi
@Temperature 71.1 °C
Parallel to Rise; ASTM D1621
 339 psi
@Temperature 71.1 °C
Perpendicular to Rise; ASTM D1621
 498 psi
@Temperature 23.9 °C
Parallel to Rise; ASTM D1621
 507 psi
@Temperature 23.9 °C
Perpendicular to Rise; ASTM D1621
Compressive Modulus 13345 psi
@Temperature 71.1 °C
Parallel to Rise; ASTM D1621
 13561 psi
@Temperature 71.1 °C
Perpendicular to Rise; ASTM D1621
 16779 psi
@Temperature 23.9 °C
Perpendicular to Rise; ASTM D1621
 17079 psi
@Temperature 23.9 °C
Parallel to Rise; ASTM D1621
Shear Modulus 1.854 ksiRise Parallel to Specimen Thickness; ASTM C273
Shear Strength 0.157 ksiRise Parallel to Specimen Thickness; ASTM C273
 
Thermal PropertiesOriginal ValueComments
CTE, linear 30.0 µin/in-°F
@Temperature -34.4 - 93.3 °C
GP Method
Thermal Conductivity 0.265 BTU-in/hr-ft²-°FASTM C518
Glass Transition Temp, Tg 225 °FASTM E1824
 
Descriptive Properties
Closed Cell Content97%ASTM D6226
Tumbling Friability (%)0.420 mins at 60 rpm, ASTM C421

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
General Plastics LAST-A-FOAM® WSF-1010 Foam
General Plastics LAST-A-FOAM® R-3325 Submersible Foam Series
General Plastics LAST-A-FOAM® FR-6710 Polyurethane Foam
General Plastics LAST-A-FOAM® FR-4510 High Density, Rigid Foam
General Plastics LAST-A-FOAM® FR-3703 Polyurethane Foam

PGENR030 / 186816

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.