MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Solvay BR® 4535A Paste Adhesive
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Description: BR® 4535A is a single component, 100% solids, aluminum filled, epoxy adhesive. It has been developed for structural bonding and applications requiring increased adhesive flexibility and impact resistance with structural service performance to 150°C (302°F). Moderate temperature cure and good shelf stability give wide application to most manufacturing locations

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.25 - 1.31 g/cc0.0452 - 0.0473 lb/in³
Solids Content 100 %100 %
Storage Temperature 4.00 °C39.2 °F
 
Mechanical PropertiesMetricEnglishComments
Tensile Modulus 3.62 GPa525 ksiYoung's, Cure Cycle: 30 minutes at 150°C (300°F)
Shear Modulus 1.04 GPa151 ksiCure Cycle: 30 minutes at 120°C (250°F)
 1.36 GPa197 ksiCure Cycle: 30 minutes at 150°C (300°F)
Shear Strength 26.2 MPa3800 psi12 months, Long term Salt Spray
 30.3 MPa4400 psiLap, 14 days 100% RH at 37°C (100°F)
 31.0 MPa4500 psiLap, 30 days Oven aging at 71°C (160°F)
 31.0 MPa4500 psi18 months, Long term Salt Spray
 32.8 MPa4760 psiInitial, Long term Salt Spray
 34.5 MPa5000 psiLap, 30 days Salt spray
 34.5 MPa5000 psi4 months, Long term Salt Spray
 34.5 MPa5000 psi8 months, Long term Salt Spray
 41.4 MPa6000 psiLap, 30 days Water immersion at 25°C (77°F)
 18.6 MPa
@Temperature -40.0 °C
2700 psi
@Temperature -40.0 °F
Lap, 30 min. at 120°C (250°F); ASTM D1002
 18.6 MPa
@Temperature 140 °C
2700 psi
@Temperature 284 °F
Lap, 30 min. at 120°C (250°F); ASTM D1002
 21.4 MPa
@Temperature 140 °C
3100 psi
@Temperature 284 °F
Lap, 30 min. at 135°C (275°F); ASTM D1002
 21.4 MPa
@Temperature 140 °C
3100 psi
@Temperature 284 °F
Lap, 30 min. at 150°C (300°F); ASTM D1002
 24.1 MPa
@Temperature -40.0 °C
3500 psi
@Temperature -40.0 °F
Lap, 30 min. at 135°C (275°F); ASTM D1002
 25.5 MPa
@Temperature 140 °C
3700 psi
@Temperature 284 °F
Lap, 60 min. at 120°C (250°F); ASTM D1002
 26.9 MPa
@Temperature 25.0 °C
3900 psi
@Temperature 77.0 °F
Lap, 30 min. at 120°C (250°F); ASTM D1002
 28.3 MPa
@Temperature -40.0 °C
4100 psi
@Temperature -40.0 °F
Lap, 30 min. at 150°C (300°F); ASTM D1002
 28.3 MPa
@Temperature -40.0 °C
4100 psi
@Temperature -40.0 °F
Lap, 60 min. at 120°C (250°F); ASTM D1002
 31.0 MPa
@Temperature 25.0 °C
4500 psi
@Temperature 77.0 °F
Lap, 30 min. at 135°C (275°F); ASTM D1002
 31.0 MPa
@Temperature 25.0 °C
4500 psi
@Temperature 77.0 °F
Lap, 30 min. at 150°C (300°F); ASTM D1002
 33.1 MPa
@Temperature 25.0 °C
4800 psi
@Temperature 77.0 °F
Lap, 60 min. at 120°C (250°F); ASTM D1002
Impact Test 5.20 J3.84 ft-lb30 days Salt spray
 5.40 J3.98 ft-lb14 days Water immersion at 54°C (130°F)
 5.70 J4.20 ft-lb30 days 100% RH at 37°C (100°F)
 5.90 J4.35 ft-lb30 days Water immersion at 25°C (77°F)
 6.30 J4.65 ft-lb30 days Oven aging at 71°C (160°F)
 4.50 J
@Temperature -40.0 °C
3.32 ft-lb
@Temperature -40.0 °F
ASTM D950
 5.40 J
@Temperature 25.0 °C
3.98 ft-lb
@Temperature 77.0 °F
ASTM D950
 6.80 J
@Temperature 140 °C
5.02 ft-lb
@Temperature 284 °F
ASTM D950
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 150 °C302 °F
Glass Transition Temp, Tg 148 °C298 °FCure Cycle: 30 minutes at 150°C (300°F)
 
Processing PropertiesMetricEnglishComments
Shelf Life 6.00 Month6.00 Month
 
Descriptive Properties
ColorGrey

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Epoxy Adhesive
Elantas EN-2523 (Conap) Potting and Encapsulation Adhesive
Solvay BR® 680-3 Polyimide Film Adhesive
Solvay VTF 261 Film
Armstrong A-2/H20 Epoxy Adhesive

PCYTED123 / 180425

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.