MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Quantum Composites QC-8700 63% Glass Fiber Reinforced Vinyl Ester SMC
Categories: Polymer; Thermoset; Composite SMC; Vinyl Ester

Material Notes: QC-8700 is a vinyl ester engineered structural composite molding compound for compression molding of components requiring high structural strength. It exhibits unusual toughness, and is suggested for applications subject to impacts and rough handling. QC-8700 is also suggested for applications requiring excellent fatigue resistance. It exhibits better temperature resistance than QC-8800.

  • Form = Rolls, Festooned Sheet
  • Color = Black, Natural
  • Glass Fiber Content = 63% nominal

A. Schulman has acquired Quantum Composites.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.87 g/cc1.87 g/ccASTM D792
Water Absorption 0.080 %0.080 %ASTM D570
Linear Mold Shrinkage 0.0010 cm/cm0.0010 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Barcol 6868ASTM D2583
Tensile Strength 344 MPa49900 psiASTM D638
Tensile Modulus 26.1 GPa3790 ksiASTM D638
Flexural Strength 585 MPa84800 psiASTM D790
Flexural Modulus 20.6 GPa2990 ksiASTM D790
Poissons Ratio 0.380.38ASTM D638
Izod Impact, Notched 17.6 J/cm33.0 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg 125 °C257 °FDMA
 
Processing PropertiesMetricEnglishComments
Processing Temperature 132 - 149 °C
@Thickness 12.7 mm
270 - 300 °F
@Thickness 0.500 in
Compression Molding
Clamp Pressure 2.07 - 6.89 MPa300 - 1000 psi
Cure Time 3.00 - 5.00 min
@Thickness 6.35 mm,
Temperature 138 °C
0.0500 - 0.0833 hour
@Thickness 0.250 in,
Temperature 280 °F
Shelf Life 2.00 Month
@Temperature 23.9 °C
2.00 Month
@Temperature 75.0 °F
 
Descriptive Properties
Fiber Length (in)1Glass, nominal

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Quantum Composites QC-7753 50% Glass Fiber Reinforced Polyester SMC
Quantum Composites QC-8777 41% Glass Fiber Reinforced Polyester Hybrid SMC
A. Schulman BMC 845 30% Glass Filled Vinyl Ester
Overview of materials for Vinyl Ester Sheet Molding Compound
A. Schulman BMC 845 Vinyl Ester Molding Compounds, 30% Glass-Filled

PCOQB902 / 139270

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.