MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Mocom (ALBIS) ALTECH® PP H ECO 4920/106 MR 20 PP, 20% Talcum
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 20% Talc Filler

Material Notes: Base Polymer: Polypropylene

Filler/Additive System: 20% talcum

Special Features: Heat ageing stabilization, contains recycled material

Market Segment: Automotive, various

Application Area: Ducting/piping systems, various

Typical Applications: Air duct, housing and automotive trim unpainted, various

Information provided by Albis Plastics

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.07 g/cc0.0387 lb/in³ISO 1183
Melt Flow 15 g/10 min
@Load 2.16 kg,
Temperature 230 °C
15 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133
Storage Temperature <= 30.0 °C<= 86.0 °Fdry, protected from light
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 22.0 MPa3190 psiISO 527
Tensile Strength 26.0 MPa3770 psiISO 527
Tensile Stress 26.0 MPa3770 psiISO 527
Elongation at Break 25 %25 %ISO 527
Elongation at Yield 6.0 %6.0 %ISO 527
Tensile Modulus 1.90 GPa276 ksiISO 527
Flexural Strength 38.0 MPa5510 psiISO 178
Flexural Modulus 2.10 GPa305 ksiISO 178
Charpy Impact Unnotched  1.00 J/cm²
@Temperature -40.0 °C
4.76 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eU
 1.20 J/cm²
@Temperature -20.0 °C
5.71 ft-lb/in²
@Temperature -4.00 °F
ISO 179/1eU
 3.00 J/cm²
@Temperature 23.0 °C
14.3 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  0.200 J/cm²
@Temperature -20.0 °C
0.952 ft-lb/in²
@Temperature -4.00 °F
ISO 179/1eA
 0.200 J/cm²
@Temperature -40.0 °C
0.952 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eA
 0.300 J/cm²
@Temperature 23.0 °C
1.43 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °C149 °FISO 75-1/-2
Vicat Softening Point 85.0 °C185 °FB50; ISO 306
Flammability, UL94 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 200 - 270 °C392 - 518 °FInjection molding
Mold Temperature 20.0 - 70.0 °C68.0 - 158 °FInjection molding
Drying Temperature  60.0 - 90.0 °C
@Time 7200 - 14400 sec
140 - 194 °F
@Time 2.00 - 4.00 hour
in a dry air (desiccant) dryer
 60.0 - 90.0 °C
@Time 7200 - 14400 sec
140 - 194 °F
@Time 2.00 - 4.00 hour
in an circulating dryer
 
Descriptive Properties
Base PolymerPolypropylene

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PALBIS8300 / 242359

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.