MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  
Master Bond adhesives
Assab Steels VANADIS 10 Cold Work Steel
Categories: Metal; Ferrous Metal; Chrome-moly Steel; Tool Steel; Cold Work Steel

Material Notes: VANADIS 4 is a chromium-molybdenum-vanadium alloyed steel which is characterized by:
  • Extremely high abrasive wear resistance
  • High compressive strength
  • Very good through-hardening properties
  • Good toughness
  • Very good stability in hardening
  • Good resistance to tempering back
  • Good Machinability
  • Simple heat treatment
  • Suitable for surface treatment

VANADIS 4 is especially suitable for very long run tooling where adhesive wear is the dominating problem. Its very good combination of extremely high wear resistance and toughness also make VANADIS 10 an interesting alternative in applications where tooling made of such materials as cemented carbide tends to chip or crack.
Examples:

  • Blanking and forming
  • Fine blanking
  • Blanking of electrical sheet
  • Gasket stamping
  • Deep drawing
  • Cold Forging
  • Slitting knives (paper and foil)
  • Powder pressing
  • Granulator knives
  • Extruder screws, etc

Vendors:
Available Properties
  • Density
  • Hardness, Rockwell C, 1020°C Austenitizing temperature, for tempering at 550°C
  • Hardness, Rockwell C, 1060°C Austenitizing temperature, for tempering at 550°C
  • Hardness, Rockwell C, Hardened and tempered.
  • Hardness, Rockwell C, 1020°C Austenitizing temperature, for tempering at 300°C
  • Hardness, Rockwell C, 1020°C Austenitizing temperature, for tempering at 500°C
  • Hardness, Rockwell C, 1060°C Austenitizing temperature, for tempering at 300°C
  • Hardness, Rockwell C, Holding time 30 minutes, Air cooling, 1000°C Austenitizing temperature
  • Hardness, Rockwell C, 1060°C Austenitizing temperature, for tempering at 500°C
  • Hardness, Rockwell C, Holding time 30 minutes, Air cooling, 1050°C Austenitizing temperature
  • Modulus of Elasticity
  • Impact Test, tempering temperature of 475°C. Specimen size: 7x10x55 mm unnotched. Hardened at 1020°C. Quenched in air. Tempered twice
  • Impact Test, tempering temperature of 275°C. Specimen size: 7x10x55 mm unnotched. Hardened at 1020°C. Quenched in air. Tempered twice
  • Impact Test, tempering temperature of 575°C. Specimen size: 7x10x55 mm unnotched. Hardened at 1020°C. Quenched in air. Tempered twice
  • CTE, linear
  • CTE, linear
  • Specific Heat Capacity
  • Thermal Conductivity
  • Thermal Conductivity
  • Thermal Conductivity
  • Carbon, C
  • Chromium, Cr
  • Iron, Fe
  • Manganese, Mn
  • Molybdenum, Mo
  • Silicon, Si
  • Vanadium, V
  
Property Data

This page displays only the text
of a material data sheet.

To see MatWeb's complete data
sheet for this material (including
material property data, metal
compositions, material suppliers,
etc
), please click the button below.

Manufacturer Notes:
none

Category Notes
none

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

 

New MatWeb Services
Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.