Gray Cast Iron, ASTM A 48 Class 40
Categories: Metal; Ferrous Metal; Cast Iron; Gray Cast Iron

Material Notes: Carbon listed in the composition table is the total carbon. Can be oil quench hardened from 860°C to attain a Rockwell C 50 minimum surface hardness. Data provided by the manufacturer, Siltin Industries, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.15 g/ccTypical for Gray Cast Iron
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 183 - 234
Hardness, Knoop 258Converted from Brinell
Hardness, Rockwell B 97Converted from Brinell
Hardness, Rockwell C 20Converted from Brinell
Hardness, Vickers 246Converted from Brinell
Tensile Strength, Ultimate >= 276 MPa
Ultimate Compressive Strength >= 1034 MPa
Machinability 0.0 %Very good machinability. No numerical rating available.
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 3.25 - 3.5 %
Chromium, Cr 0.050 - 0.45 %
Copper, Cu 0.15 - 0.40 %
Iron, Fe 91.9 - 94.2 %As Balance
Manganese, Mn 0.50 - 0.90 %
Molybdenum, Mo 0.050 - 0.10 %
Nickel, Ni 0.050 - 0.20 %
Phosphorus, P <= 0.12 %
Silicon, Si 1.8 - 2.3 %
Sulfur, S <= 0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.